Carbon equivalent calculator (CE, Pcm, CET) and preheat

Weldability of steel from its composition: IIW carbon equivalent, AWS CE with silicon, Pcm and CET, with the EN 1011-2 minimum preheat temperature.

Units

Results are estimates. They do not replace the governing code, class or flag requirements, or a check by a competent person. Report a problem

Introduction

When steel is welded, the heat-affected zone cools fast and can harden. Hard zones with hydrogen from the weld can crack hours after welding. The carbon equivalent rolls carbon and the alloying elements into one number that measures this hardenability. The S355 plate of the worked example has a CE of 0.44, and at 30 mm thickness it needs about 110 °C of preheat by EN 1011-2.

This calculator gives four carbon equivalents from the mill certificate: the IIW CE, the AWS D1.1 version with silicon, Ito and Bessyo's Pcm, and the CET of EN 1011-2. With the plate thickness, the hydrogen level and the heat input, it also gives the minimum preheat temperature by EN 1011-2 method B. It is for welding engineers, inspectors and fabricators writing or checking a welding procedure.

Formulas

Carbon equivalents, with element contents in mass %:

CE(IIW) = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15
CE(AWS) = C + (Mn + Si)/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15
Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5 B
CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40

Minimum preheat, EN 1011-2 Annex C, method B:

T_p = 697 CET + 160 tanh(d/35) + 62 HD^0.35 + (53 CET − 32) Q − 328    °C
  • d — plate thickness, mm (10 to 90)
  • HD — diffusible hydrogen of the weld metal, ml/100 g (1 to 20)
  • Q — effective heat input, kJ/mm (0.5 to 4.0): arc energy times the thermal efficiency of the process
  • The formula holds for CET 0.20 to 0.50 % and C 0.05 to 0.32 %, Mn 0.5 to 1.9 %, Si up to 0.8 %, Cr up to 1.5 %, Cu up to 0.7 %, Mo up to 0.75 %, Ni up to 2.5 %, V up to 0.18 %, Nb up to 0.06 %, Ti up to 0.12 % and B up to 0.005 %

Assumptions and limitations

  • The composition comes from the mill certificate. An element left at zero counts as absent, which understates the result if it is actually there.
  • CE(IIW) suits carbon and carbon-manganese steels. Pcm was derived for low-carbon, low-alloy steels such as modern pipeline grades, where CE(IIW) is less reliable.
  • The preheat is the minimum to avoid hydrogen cracking. Restraint, hardness limits and the governing code may require more, and the calculator refuses inputs outside the validity range of the formula.
  • Heat input Q must already include the thermal efficiency of the process. EN 1011-1 gives the efficiency factors.

Worked example

An S355 plate 30 mm thick has C 0.18, Mn 1.40, Si 0.30, Cr 0.05, Mo 0.02, V 0.01, Ni 0.05 and Cu 0.10 %. It is welded with consumables of HD 5 ml/100 g at an effective heat input of 1.0 kJ/mm.

  1. CE(IIW) = 0.18 + 0.2333 + 0.016 + 0.010 = 0.439.
  2. CE(AWS) adds 0.30/6 = 0.05: 0.489.
  3. Pcm = 0.18 + 0.010 + 0.0775 + 0.0008 + 0.0013 + 0.001 = 0.271.
  4. CET = 0.18 + 0.142 + 0.0075 + 0.0013 = 0.331.
  5. Preheat: 697 × 0.331 + 160 tanh(30/35) + 62 × 5^0.35 + (53 × 0.331 − 32) × 1.0 − 328 = 108 °C.

So this joint needs a preheat of at least 110 °C. Thinner plate, lower-hydrogen consumables or a higher heat input would lower it.

FAQ

What is the carbon equivalent of steel?

A single number that weighs carbon and the alloying elements by their effect on hardenability. The higher it is, the more the heat-affected zone hardens and the greater the risk of cold cracking.

Which carbon equivalent formula should I use?

The one your code names. EN 1011-2 uses CE or CET, AWS D1.1 uses CE with silicon or Pcm, and pipeline specifications often give a limit on Pcm.

What CE value needs preheat?

There is no single limit, because thickness, hydrogen and heat input matter as much. Use a method such as EN 1011-2, which combines all of them.

What is diffusible hydrogen HD?

The hydrogen that the weld metal releases after welding, in ml per 100 g of deposited metal. Consumables are classified by it: H5 means at most 5 ml/100 g, H10 at most 10.

Why does a higher heat input lower the preheat?

More heat slows the cooling of the joint. The heat-affected zone hardens less and hydrogen has more time to escape.

Can I use these formulas for stainless steel?

No. Austenitic stainless steels do not harden this way, and their weldability is judged by other means such as the ferrite content.

Related calculators

What this calculator is checked against

Before every release the calculator must reproduce each case below. The note under each case says where the expected answer comes from: a standard, a textbook, a published table, or a hand calculation shown in full.

  1. C-Mn steel C 0.18, Mn 1.40, Si 0.30, Cr 0.05, Mo 0.02, V 0.01, Ni 0.05, Cu 0.10: CE 0.4393, CE(AWS) 0.4893, Pcm 0.2707, CET 0.3308EN 1011-2 Annex C (CE, CET); AWS D1.1 Annex B (CE + Si/6); Ito–Bessyo Pcm (hand calculation)
  2. Plain carbon steel C 0.20, Mn 0.60: CE = 0.20 + 0.10 = 0.30, Pcm = 0.20 + 0.03 = 0.23, CET = 0.20 + 0.06 = 0.26Formulas of EN 1011-2 Annex C and Ito–Bessyo (hand calculation)
  3. EN 1011-2 C.3 preheat: CET 0.35 %, d 20 mm, HD 2, Q 1.5 kJ/mm gives 57.4 °C; the example gives 108.1 °CT_p = 697 CET + 160 tanh(d/35) + 62 HD^0.35 + (53 CET − 32) Q − 328 (EN 1011-2 Annex C, method B; hand calculation)
  4. Preheat trends: thicker plate and more hydrogen need more preheat, a higher heat input needs lessEN 1011-2 Annex C: the effects of d, HD and Q on the minimum preheat
  5. Each element enters with its coefficient: 0.5 % Ni adds 0.0333 to CE, 0.0083 to Pcm and 0.0125 to CET; 0.002 % B adds 0.01 to Pcm onlyCoefficients of CE(IIW), Pcm and CET
  6. Outside EN 1011-2 method B: Mn 0.3 %, C 0.40 %, 5 mm plate, HD 30 and Q 5 kJ/mm are refused; CE alone still calculatesEN 1011-2 Annex C validity range (C 0.05–0.32, Mn 0.5–1.9 %, d 10–90 mm, HD 1–20, Q 0.5–4.0)
  7. Worked example of the article: the calculator reproduces 0.439, 0.489, 0.271, 0.331, 108 °C to the digits printedThe worked example on this page, to the digits printed

Assumptions and sources

Assumptions and limits

  • Element contents are mass per cent from the mill certificate (heat or product analysis). Elements left at zero are taken as absent, which can understate the carbon equivalent if they are present.
  • CE(IIW) suits carbon and carbon-manganese steels; AWS D1.1 adds Si/6 to it. Pcm (Ito and Bessyo) was derived for low-carbon low-alloy steels, where CE(IIW) is less suitable. CET is the carbon equivalent of EN 1011-2 method B.
  • The preheat temperature uses the formula of EN 1011-2 Annex C method B and is given only within its validity range: CET 0.20 to 0.50 %, thickness 10 to 90 mm, diffusible hydrogen 1 to 20 ml/100 g, heat input 0.5 to 4.0 kJ/mm, and the composition limits of that annex. Outside it the calculator refuses rather than extrapolates.
  • The preheat is the minimum to avoid hydrogen cold cracking in the heat-affected zone of a butt weld; restraint, hardness limits, the welding procedure and the governing code may require more. Heat input Q here is the effective value (arc energy × thermal efficiency).

Sources

  • EN 1011-2:2001, Welding — Recommendations for welding of metallic materials — Part 2: Arc welding of ferritic steels, Annex C (method A, CE; method B, CET and preheat equation C.3)
  • AWS D1.1/D1.1M:2025, Structural Welding Code — Steel, Annex B (alternative methods for determining preheat; CE with Si/6 and Pcm)
  • Ito, Y. and Bessyo, K. (1968), Weldability formula of high strength steels related to heat-affected zone cracking, IIW Doc. IX-576-68 (Pcm)
  • TWI, FAQ: What is the difference between the various carbon equivalent formulae used in relation to hydrogen cracking?

Cite this calculator

Papandreou, C. (2026). Carbon equivalent calculator (CE, Pcm, CET) and preheat. Engineering Bible. https://engineeringbible.com/mechanical/carbon-equivalent/