Skip to content
Engineering Bible

Results appear as you type. Use the arrow keys to move through them and Enter to open one.

Popular

↑ ↓ moveEnter openEsc close

Hardness conversion calculator (HRC, HRB, HV, HB)

Approximate conversion of steel hardness between Rockwell C, Rockwell B, Vickers and Brinell, with tensile strength, from ASTM E140 and ISO 18265.

Units
Leer en español

Results are estimates. They do not replace the governing code, class or flag requirements, or a check by a competent person. Report a problem

Introduction

Each hardness test presses a different indenter into the metal with a different load, so the scales have no exact relation. For steel, standard tables built from many paired tests give the equivalent values. A steel at 45 HRC reads about 446 HV and 421 HBW, and its tensile strength is roughly 1 440 MPa.

This calculator converts a reading in Rockwell C, Rockwell B, Vickers or Brinell to the other scales, and estimates the tensile strength. It can also work backwards from a tensile strength. It interpolates in the published tables and refuses values outside them. It is for inspectors, heat-treaters and designers comparing a hardness test with a drawing or a material certificate.

Formulas

Hardness to hardness, by linear interpolation between two rows of ASTM E140:

y = y₁ + (x − x₁) (y₂ − y₁) / (x₂ − x₁)
  • x — the reading you have; x₁, x₂ — the table rows either side of it
  • y₁, y₂ — the values of the other scale in those rows

Tables used:

RangeTableColumns
HRC 20 to 68ASTM E140 Table 1HRC, HV, HBW (carbide ball, 3 000 kgf)
HRB 55 to 100ASTM E140 Table 2HRB, HV, HB (equal to HV in this range)
HV 80 to 650ISO 18265 Table A.1HV, tensile strength Rm 255 to 2 180 MPa

The Vickers number links the tables: every reading is first converted to HV, then to the other scales and to the tensile strength.

Assumptions and limitations

  • The tables hold for non-austenitic carbon and low-alloy steels. Austenitic stainless steel, cold-worked steel, cast iron, aluminium and copper alloys need their own tables.
  • Rockwell C stops at 20 HRC and Rockwell B at 100 HRB. Below 20 HRC use Rockwell B; above 100 HRB use Rockwell C.
  • Where Table 1 meets Table 2, around 98 to 100 HRB, the two tables differ by up to 10 HV. Conversions in that band are less certain.
  • The tensile strength is only an estimate. ISO 18265 calls it the least reliable of the converted values.
  • A converted value never replaces a test in the scale a specification asks for. ASTM E140 itself says to convert only when testing in that scale is not possible.

Worked example

A heat-treated shaft of alloy steel tests at 45 HRC. What are its Vickers and Brinell hardness and its approximate tensile strength?

  1. ASTM E140 Table 1, row 45 HRC: 446 HV and 421 HBW.
  2. ISO 18265 Table A.1: 440 HV is 1 420 MPa and 450 HV is 1 455 MPa.
  3. Interpolate at 446 HV: 1 420 + 0.6 × 35 = 1 441 MPa.

So the shaft is about 446 HV, 421 HBW and 1 441 MPa. The older SAE tensile column printed with E140-based charts gives 1 480 MPa for 45 HRC, within 3 % of this estimate.

A softer plate at 85 HRB converts the same way through Table 2: 165 HV, 165 HB and about 530 MPa.

Common cases

Rockwell C hardness from 25 to 55, the range of most quenched-and-tempered carbon and alloy steel parts, converted to Vickers and Brinell with an estimated tensile strength. Steels only: stainless, cast iron and non-ferrous metals need their own tables.

CaseVickers, HVBrinell, HBWTensile strength, approx. (MPa)
HRC 25266253853
HRC 30302286971
HRC 353453271,110
HRC 403923711,262
HRC 454464211,441
HRC 505134811,676
HRC 555955601,975

Every row is worked out by this calculator each time the site is built, and checked for impossible values. Open a case to load its inputs.

Common mistakes

  • Using the steel tables for other metals. Austenitic stainless steel, aluminium, brass and cast iron work-harden and deform differently under the indenter, so a steel conversion can be off by a whole hardness grade. Use the table for that material, or test in the scale you need.
  • Converting a surface reading into a core strength. A case-hardened, nitrided or decarburised part has a surface unlike its core. The tensile estimate from a surface reading describes neither.
  • Testing a round part without the curvature correction. On a convex cylinder the indenter sinks further and Rockwell reads low. Below about 25 mm diameter, add the correction from ASTM E18 or ISO 6508 before converting.
  • Testing thin material. The test piece should be at least about ten times as thick as the indentation is deep, or the anvil shows through and the reading is too high.
  • Treating the converted value as a test result. When a specification calls for hardness in one scale, a value converted from another scale does not show compliance. ASTM A370 and ISO 18265 both say so.

FAQ

Can I convert HRC to HRB?

Only near the top of the B scale. 20 HRC is about 99.7 HRB, and the B scale ends at 100 HRB, so harder steels have no HRB value.

How do I convert Brinell to Rockwell C?

Find the Brinell number in E140 Table 1 and read the HRC in the same row. For example, 400 HBW is 43 HRC.

How accurate are hardness conversions?

They are approximate. ASTM E140 warns that converted values may be inaccurate for a given material, and ISO 18265 treats the tensile estimate as the least reliable.

Why is there no tensile strength above 650 HV?

ISO 18265 Table A.1 stops at 650 HV and 2 180 MPa. Harder steels are brittle, and their tensile strength depends more on defects than on hardness.

Does this work for stainless steel?

Not for austenitic grades such as 304 and 316. ASTM E140 gives austenitic stainless steel a table of its own.

What is the difference between HB and HBW?

HBW means the test used a tungsten carbide ball. Older tests with a steel ball were marked HBS; modern standards allow only the carbide ball.

Related calculators

What this calculator is checked against

Before every release the calculator must reproduce each case below. The note under each case says where the expected answer comes from: a standard, a textbook, a published table, or a hand calculation shown in full.

  1. E140 Table 1 rows: 60 HRC = 697 HV, 654 HBW; 50 HRC = 513 HV, 481 HBW; 40 HRC = 392 HV, 371 HBW; 30 HRC = 302 HV, 286 HBWASTM E140 Table 1 (non-austenitic steels, Rockwell C range)
  2. E140 Table 2 rows: 100 HRB = 240 HV, 90 HRB = 185 HV, 80 HRB = 150 HV, 60 HRB = 107 HV (HB = HV in this range)ASTM E140 Table 2 (non-austenitic steels, Rockwell B range)
  3. Inverse and interpolation: 446 HV gives 45.0 HRC; 400 HBW gives 43.0 HRC; 45.5 HRC lies half-way between 446 and 458 HVASTM E140 Table 1, linear interpolation between rows (by hand)
  4. ISO 18265 tensile strength: 446 HV (45 HRC) ≈ 1 441 MPa; 165 HV (85 HRB) = 530 MPa; 800 MPa ↔ 250 HVISO 18265 Table A.1 rows (440 HV 1 420 MPa, 450 HV 1 455 MPa, 165 HV 530 MPa, 250 HV 800 MPa)
  5. Spot-check against a second table: ISO 18265 tensile within 3 % of the SAE/ASTM tensile column (1 480 MPa at 45 HRC, 950 MPa at 30 HRC)Miki Pulley technical data, Rockwell C hardness conversion table (approximate tensile strength column)
  6. Out of the tables: HRC 18, HRB 105, HV 950 and 3 000 MPa are refused; 68 HRC has no Brinell or tensile valueBehaviour check: warnings and rejected inputs
  7. Worked example of the article: the calculator reproduces 446, 421, 1 441 MPa to the digits printedThe worked example on this page, to the digits printed

Assumptions and sources

Assumptions and limits

  • The conversions apply only to non-austenitic carbon and low-alloy steels, in the heat-treated, hot-rolled or annealed condition the tables were built from. Austenitic stainless steel, cold-worked steel, cast iron and non-ferrous metals need their own tables.
  • Hardness numbers are converted with ASTM E140 Table 1 (Rockwell C range, HRC 20 to 68) and Table 2 (Rockwell B range, HRB 55 to 100), interpolating linearly between rows. Brinell is the 10 mm tungsten carbide ball at 3 000 kgf (HBW).
  • Tensile strength is estimated from the Vickers number with ISO 18265 Table A.1 (HV 80 to 650, Rm 255 to 2 180 MPa). ISO 18265 warns that tensile estimates are the least reliable converted values.
  • E140 Tables 1 and 2 meet at about HRB 97 to 100 and HRC 20 to 23 and disagree there by up to about 10 HV; conversions in that band are less certain.
  • Values outside a table are refused or shown as "—", never extrapolated. A converted hardness never replaces a test in the scale a specification requires.

Sources

  • ASTM E140-12b(2019)e1, Standard Hardness Conversion Tables for Metals, Table 1 (non-austenitic steels, Rockwell C range) and Table 2 (Rockwell B range)
  • ISO 18265:2013, Metallic materials — Conversion of hardness values, Annex A, Table A.1 (unalloyed and low-alloy steels and cast steel)
  • ASTM A370-24, Standard Test Methods and Definitions for Mechanical Testing of Steel Products, §17 and Tables 3–4 (use of hardness conversions)

Cite this calculator

Papandreou, C. (2026). Hardness conversion calculator (HRC, HRB, HV, HB). Engineering Bible. https://engineeringbible.com/mechanical/hardness-conversion/

Embed this calculator on your site

Copy this HTML into your page. The calculator stays free to use and links back here.

By Christos Papandreou. Updated . How the numbers are checked.